In
300-mm semiconductor fabrication there is a trend toward the use of
single-wafer postetch polymer wet cleans for copper/low-k polymer stacks.
These cleaning steps pose a number of challenges, such as how to successfully
clean the low-k stacks without adversely affecting the properties of
the low-k film or the underlying materials, and how to mitigate damage
to the interconnect metal. For organic low-k films, potential integration
problems include the compatibility of clean chemistries with integrated
adhesion promoters and excessive swelling of the low-k film itself.
The biggest problem facing the interconnect metal is its potential to
experience surface corrosion. The successful introduction of porous
low-k materials will depend on how effectively these issues can be addressed.
The
purpose of the study described in this article was to evaluate the impact
of a single-wafer postetch cleaning tool on porous SiLK dielectric resin
films manufactured by Dow Chemical (Midland, MI). The article focuses
on the relationship between different chemical process approaches and
the resulting electrical characteristics of cleaned structures. The
electrical test characterization results presented here show that a
single-wafer cleaning step, depending on the particular chemistry formulation
used, can improve the performance of selected test devices by lowering
line resistance (R) and increasing capacitance (C). The data show that
an appropriate chemical clean can result in electrical RC product performance
that is as good as or better than that of the non-wet-clean process
of record (POR).
Experimental
Procedure
The
test vehicle used in these experiments was a single-damascene structure.
The structure consisted of an integrated stack that had a porous dielectric
film capped with an SiC/SiO2 dual hard mask. The
minimal lithographic target had a 175-nm linewidth and 0.225-µm
spacing. The smallest linewidth was 140 nm. Patterning was achieved
using 193-nm lithography combined with an H2/N2
reactive ion etch. The postetch trench height was ~100 nm; trench pitch
was 3:1. The etch step incorporated an in situ resist removal procedure,
thus eliminating the need for a separate resist ash step. The etch chemistry
used resulted in the deposition of a protective sidewall polymer, which
had to be removed by means of a wet clean.
The
experiments were performed on a single-wafer spin processor from SEZ
(Villach, Austria). Three different chemistries were investigated for
the postetch cleaning step, each representing a fundamentally different
approach to residue removal. Chemistry 1 is a commercially manufactured
aqueous organic (carboxylic) acid mixture. Chemistry 2, also a commercially
manufactured organic mixture, is a more traditional solvent-based product.
Chemistry 3 was developed in-house at SEZ using dilute acid ingredients.
It was composed of >>99% DI water.
The
chemistries' compatibility with the dielectric film was evaluated by
determining the characteristics of blanket dielectric films. Their cleaning
effectiveness was determined by tilt scanning electron microscopy (SEM)
analysis. Based on the results of that analysis, best-known-method (BKM)
conditions were ascertained for each chemistry. These BKMs were used
for processing blanket and porous dielectric film structures and materials
and for probing their electrical properties.
Experimental
Results
Processing
the Blanket Dielectric Films. After the blanket dielectric
films were processed using the three chemistries, a bake step was performed
to remove a spurious peak associated with outgassing from the wafer
carrier. Then infrared (IR) spectroscopy was conducted to determine
whether the films' chemical structure had changed. The IR data indicated
that chemical processing did not change the films significantly and
did not add chemical species such as water. The physical and electrical
properties of the blanket dielectric films are summarized in Tables
I and II. The data in
the tables are consistent with the target values for porous dielectric
films and the IR results.
 |
| Table
I: Film-thickness variation and adhesion data of porous low-k material
after wet clean. |
SEM
Analysis. Figure 1 presents tilted SEM images of similar serpentine
locations on different wafers, illustrating the effects of the different
wet clean chemistries on the device structure. Figure 1a, the result
of the baseline process, illustrates an as-etched wafer region that
received no further postetch treatment. It was apparent that polymer
residue had been removed from both the SiCN (hard-mask) layer and the
etched porous dielectric film sidewalls. Furthermore, there was no visible
evidence that polymeric residue was present on the underlying SiCN layer.
 |
| Figure
1: SEM images showing a serpentine structure processed (a) without
postetch chemical cleaning, (b) with chemistry 1, (c) with chemistry
2, and (d) with chemistry 3. |
There
was less sidewall residue on the structures shown in Figures 1b–1d
than on the structure in Figure 1a, but in all cases, the sidewalls
displayed a significant mottling effect, which was associated with the
use of the 193-nm resist. There appeared to be a similar amount of sidewall
residue on the wafers processed using chemistries 1 (Figure 1b) and
2 (Figure 1c), and in both cases there was no apparent evidence of residue
on the underlying SiCN layer.
While
the wafers processed using chemistry 3 displayed somewhat less residue
on the porous dielectric film sidewalls and SiCN layers than did the
wafers processed using chemistries 1 and 2, there was an artifact on
the underlying SiCN layer that is clearly visible in Figure 1d. That
artifact had two possible origins. First, chemistry 3 could have reacted
with the SiCN layer, causing bubbling or delamination. However, given
the nature and concentrations of the components in chemistry 3, that
explanation is highly unlikely, since the mixture did not react noticeably
with any of the underlying films. Second, the artifact could have been
caused by polymer residue located on the SiCN surface at the bottom
of the trench. Since that residue could not have been deposited by the
chemical filtration and dispense system used in the experiments, it
was concluded that a uniform residue, not readily apparent in the SEM
image in Figures 1a–1c, was present on the open areas of the underlying
SiCN film. Under the given process conditions, that residue had been
attacked and partially removed by chemistry 3. Visual evidence provided
by SEM analysis and supported by subsequent parametric data substantiates
that conclusion.
Parametric
Evaluation. Figure
2a shows the cumulative resistance distribution of a 2850-cm-long
M1 serpentine with a 0.175-µm line and 0.225-µm space, while
Figure 2b shows the cumulative
resistance distribution of a 0.32-cm-long isolated serpentine with a
9.0-µm line and a 1.0-µm space. The data presented in these
figures are consistent with the effects of the different chemistries
shown in the SEM images in Figure 1. While there is a barely distinguishable
difference between the data for wafers processed using the baseline
chemistry and chemistry 2, indicating that they did not remove sidewall
polymer during wet cleaning, the data for the wafers processed using
chemistries 1 and 3 show a clear decrease in line resistance, reflecting
their ability to remove the sidewall polymer. Chemistries 1 and 3 outperformed
chemistry 2 because they were also able to remove the residual polymer
from the bottom of the SiCN trench, thereby maximizing the copper line
cross-sectional area.
 |
| Figure
3: Relative resistance change as a function of residue thickness.
|
The
relative effect of overall polymer residue on line resistance is shown
in Figure 3. Based on an analysis of median resistance values derived
from the electrical data in Figure 2a, a decrease in resistance of approximately
6% was observed, corresponding to a sidewall polymer thickness of approximately
4 nm. That estimate is similar to the actual residue thickness that
was measured during cross-sectional analysis.
Interline
capacitance data from 400-µm-long comb fingers with a 0.175-µm
line and a 0.225-µm space are presented in Figure 4. In general,
the more polymer residue that was removed, the more capacitance increased.
The chemistries that had the greatest impact on line resistance—1 and
3—also had the greatest impact on capacitance. Capacitance on the wafers
that had been processed using chemistries 1 and 3 was 6% greater than
that on the wafers processed using the baseline application or chemistry
2.
 |
| Figure
4: Interline capacitance of 400-µm-long comb fingers with a
0.175-µm line and a 0.225-µm space. |
To
investigate the effect of polymer residue on capacitance, a 2-D Raphael
simulation model was built. Figure 5 presents the results of that simulation
for the wafers that were processed using chemistry 3, which removed
residue from the sidewalls and bottom of the trench. While the Raphael
simulation model did not permit the investigators to determine the precise
k-value of the polymer residue within the model's error limits, it did
show that a relative change in capacitance of 6% corresponded to the
removal of approximately 3 nm of polymeric residue from the sidewalls
and bottom of the device structure. Despite the model's limitations,
that value was within the model's expected error range and matched actual
residue-thickness measurements.
 |
| Figure
5: Simulated capacitance change as a function of residue thickness.
|
Finally,
RC line delay was computed using the line resistance and interline capacitance
data obtained for each chemistry. As illustrated in Figure 6, chemistry
3 provided the lowest RC delay, which was consistent with resistance
and capacitance results and was within the error limits of the measurements.
Conclusion
This
article presents the results of experiments to determine the effects
of single-wafer cleans on porous dielectric-film wafer stacks. It demonstrates
that the physical and electrical properties of selected devices containing
porous low-k material can be improved by using an appropriate wet cleaning
chemistry to remove post-dry-etch residue. Furthermore, it shows that
an in-house dilute-acid cleaning mixture appears to result in equivalent
or better device performance than commercial organic mixtures. The in-house
formulation also provides an unmatched cost of ownership.
 |
| Figure
6: RC delay, computed using the line resistance and interline capacitance
data for each chemistry. |
The
cleaning efficiency of the in-house chemistry resulted in the removal
of polymer residue from sidewalls and the bottom of trenches. From both
physical and parametric electrical analysis, it was determined that
a 3- to 4-nm layer of polymer residue present on the sidewalls and bottom
of the trench was effectively removed, resulting in improved overall
RC performance. The observed change in the cross-sectional area of the
device structures was sufficient to account for the improvement in electrical
resistance and capacitance values.
In
conclusion, the method described here provides customers with a means
to derive greater value from the use of SiLK dielectric resin.
Acknowledgments
The
authors would like to express their appreciation for the support provided
by Steve Rozeveld, Elvin Beach, and Charlie Wood at Dow Chemical Analytical
Sciences. They would also like to thank Gale Hansen of SEZ for generating
the SEM data presented in this article. Special thanks go to Brent Ames,
Frank Tolic, and Vangie Lopez at International Sematech's wafer services
for the electrical test data discussed here.
Leo
Archer, PhD, serves as director of emerging
technologies at SEZ in Phoenix. He joined SEZ America in 1999 as the
lead process engineer responsible for the development of a new hybrid
cleaning product. Appointed senior technologist in 2002, he furthered
SEZ's work with low-k materials and etch-residue removal applications.
Before joining the company, Archer worked for Intel and TI in the CMP
area and on novel device development and advanced cleaning processes.
He has written many papers and articles for scientific and industry
publications. He received a BS in chemistry and a PhD in inorganic chemistry
from the University of New Mexico in Albuquerque. (Archer can be reached
at 602/453-5023 or larcher@us.sez.com.)
Joost
Waeterloos, PhD, is responsible for leading the integration
of advanced materials and the coordination of research consortia programs
at Dow Chemical, which he joined in 1998. He has published more than
45 papers in the field of low-k integration, holds four patents on copper
dual-damascene architecture, and has written a book chapter on integration.
Waeterloos received a master's degree in electrical engineering in 1991
and a master's degree in microelectronic engineering in 1994 from the
University of Leuven, Belgium. In 1998 he received a PhD from the University
of Leuven for research on integration of low-permittivity dielectrics
in advanced interconnect technologies. (Waeterloos can be reached at
+32 476 313086 or jwaeterloos@dow.com.)
Michael
Simmonds, PhD, joined the advanced electronic materials business
unit of Dow Chemical in 1997 and has been leading projects to evaluate
new polymers for electronic applications. In 2001, he was appointed
SiLKnet Alliance development manager. Simmonds has held several positions
at Elf Atochem, the Swiss Center of Microtechnology, and Dow Chemical
focusing on the application of new materials to a variety of high-tech
fields. His work has been published in the scientific and patent literature,
and he is also the author of a book chapter. Simmonds received a bachelor's
degree in chemistry from the University of Surrey, Guildford, UK, in
1988. In 1993, he received a PhD based on his advanced studies in the
area of low-temperature aluminum chemical vapor deposition, which he
carried out at the Center for Interfacial Engineering with support from
the University of Minnesota in Minneapolis. (Simmonds can be reached
at +11 411 7282642 or msimmonds@dow.com.)
Brent
Ames has managed the sales and marketing group of the advanced
technology development facility at International Sematech for the past
four years. He has worked in Sematech's CVD, etch, photolithography,
and diffusion divisions for seven years. Before beginning semi- conductor
research at Sematech, Ames worked for the IBM RISC 6000 division. He
received a bachelor's degree in business management from St. Edwards
University in Austin, TX. (Ames can be reached at 512/356-7021 or brent.ames@sematech.org.)
Frank
Tolic heads wafer services back-end product integration at
International Sematech. Previously, he worked as project manager for
technology transfer of copper low-k with a member company and as product
engineer for interconnect thrust for Sematech. Before that, Tolic worked
for GM, Ford, and Chrysler. Additionally, he worked at Motorola for
seven years as a device engineer in the advanced products research and
development laboratory, which included work on the first copper-based
IC product. The coauthor of several industry papers, he received bachelor's
degrees in electrical engineering and mechanical engineering from Lawrence
Tech University in Southfield, MI. (Tolic can be reached at 512/356-3340
or frank.tolic@sematech.org.)
Ketan
Itchhaporia worked for Dow Chemical as an application development
and technical sales engineer for spin-on dielectric materials until
February 2004. Previously, he held positions as a senior process development
engineer and technical sales engineer at FSI International in the area
of coater/developer and spin-on dielectric tracks equipment. Itchhaporia
has more than 14 years of experience in semiconductor manufacturing,
including experience in bringing products from concept to production,
conducting equipment process demonstrations for customers, and sales
and production support. He received a bachelor's degree in chemistry
(industrial electronics and electrochemistry) from the Gujarat University
in Ahnedabad, India, and completed a business management program at
the H.B. Institute of Communication & Management in Ahnedabad. (Itchhaporia
can be reached at 510/468-9359 or gkfly@aol.com.)